2013-10-31Аннотация:
Ceramic semiconductor SnO2-based materials with MnO2 and CuO additives were synthesized at
1300 ºС and 1400 ºС. There has been carried out an investigation of the physical–mechanical and
high–temperature electric properties. As a result, sintering of the material with MnO2 additive is
shown to be improved at increasing firing temperature. The composition 96 % SnO2-2 % Sb2O3-2 %
CuO made at the temperature 1300 ºС has the best electrophysical properties (its resistivity is 0.09
mOhm m). The resistivity of the 94 % SnO2-2 % Sb2O3-2 % CuO-2 % MnO2 composition in the hightemperature
region is more by a factor of 3. The 96 % SnO2-2 % Sb2O3-2 % MnO2 composition has
nonlinear voltage-currant characteristic, and hysteresis is present Синтезированы керамические полупроводниковые материалы на основе диоксида олова с
добавками MnO2 и CuO. Температуры синтеза были 1300 и 1400 ºС. Проведены исследования
физико-механических и электрофизических свойств. Показано, при повышении температуры
обжига для материала, полученного при использовании MnO2, происходит существенное
улучшение спекания. Наилучшими электрофизическими характеристиками обладают образцы
состава 96%SnO2-2%Sb2O3-2%CuO полученные при температуре обжига 1300 ºС(УЭС 0,09
мОм×м). УЭС состава 94%SnO2-2%Sb2O3-2%CuO-2%MnO2 в высокотемпературной области
выше в 3 раза. Для состава 96%SnO2-2%Sb2O3-2%MnO2 вольтамперная характеристика имеет
нелинейный вид и присутствует гистерезис